H2S Corrosion in Covers and Ducts: Material Selection

Choosing an H2S corrosion duct material comes down to three conditions, in this order: whether the gas is wet, how hot it runs, and whether chlorides are present. Wet gas rules out carbon steel. Above 80°C it rules out most plastics. Chlorides above roughly 200 mg/L rule out 316L. Meet all three and a vinyl ester FRP, or polypropylene on a cool stream, covers most odour systems on a treatment plant.

Stainless steel odour treatment cabinets with inspection windows, flanged ductwork, a stack and a control panel on a roof
Stainless cabinets, flanged duct and a stack on one roof. Stainless looks like the safe answer. On a warm, chloride-bearing odour stream it is often the shortest-lived choice.

Dry H2S is a different problem from wet H2S

Hydrogen sulfide on its own is a weak acid and a modest corrodent. What destroys equipment is the water film it dissolves into. Once that film forms on steel or concrete, the acid sits against the surface instead of passing through. The corrosion rate then jumps.

So the first question is not the concentration. It is whether the gas will condense. A duct at 200 ppm and 45°C with no condensation will outlast a duct at 5 ppm and 25°C that runs wet all year. The second one keeps a fresh acid film on the wall.

On a treatment plant, almost every odour stream is saturated. Covers sit above warm liquid. Scrubber outlets carry droplets. Extraction air cools on its way to the roof and drops below its dew point somewhere along the run. Treat condensation as certain and choose accordingly, unless you can show a measured dew point well below the duct temperature.

Aerial view of concrete treatment basins with aerated blue water, equipment buildings and walkways
One plant, several gas conditions. The headspace above a covered channel, the air from a scrubber outlet and the room air of a dewatering hall each need a different answer.

Where the corrosion actually happens

Concrete is the material people underestimate. The damage does not happen under water. It happens in the moist headspace above the waterline, on the underside of a cover and on the upper walls of a wet well.

The sequence has two stages. Hydrogen sulfide dissolves into the moisture film and reacts with the calcium hydroxide in the cement. Then sulfur-oxidising bacteria colonise the surface and turn the absorbed sulfide into sulfuric acid. That acid converts calcium hydroxide into gypsum and ettringite, both of which take up more space than the material they replace. The concrete cracks from the inside, and the surface turns soft and pasty.

The rate is not academic. Reported loss runs from 1 to 5 mm of concrete a year, and severe cases reach 10 mm. A structure designed for 75 years can lose its cover layer in a decade. The bacteria work hardest below pH 2, and the surface pH falls from its natural 11 to 12 down to 4 or 5 before they settle in.

Concrete basin walls with visible waterline staining above the liquid level and steel handrails along the rim
Concrete basin walls with a marked waterline. The staining above the liquid is where the acid film sits, and it is the first place to inspect for softening.
The 0.1 ppm threshold US EPA guidance puts the threshold for sulfide-induced corrosion of concrete near 0.1 ppm in the headspace. That is far below the odour threshold and far below any occupational limit. A plant can pass every smell complaint and still be eating its own structures.

How to pick an H2S corrosion duct material

Work through the three questions one at a time. Each one eliminates options, and the survivor is usually obvious by the third.

Step 1
Is the gas wet?
Saturated or condensing → eliminate carbon steel and standard coated steel. Move to step 2. Dry and provably below dew point → coated carbon steel is viable, but verify with a measurement, not an assumption.
Step 2
How hot does it run?
Under 60°C → PVC is possible. 60 to 80°C → PP-H is the default. 80 to 120°C → vinyl ester FRP. Above 120°C → 316L or a lined steel, and check the resin limit.
Step 3
Any chlorides or other acids?
Chloride above about 200 mg/L → drop 316L, move to duplex or a plastic. HCl or HF present → plastics win, and HF rules out glass-reinforced anything.
The combination that covers most odour work: PP-H below 80°C, vinyl ester FRP from 80 to 120°C, and duplex stainless only where heat, pressure or abrasion forces metal.

Covers need the same treatment as ducts

The title of the problem says covers, and it is worth saying plainly: a cover lives in the worst position on the plant. It sits directly above warm liquid, on its underside it sees saturated gas at full concentration, and on its top side it takes sun, rain and foot traffic. Both faces need a material decision.

GRP is the usual answer for new covers, and for good reason. It does not corrode in the headspace, it weighs a fraction of concrete, and it can span a channel without heavy steel. The limits are ultraviolet degradation on the top face and deflection under snow or maintenance load. Specify a UV-stable gelcoat, and check the panel span against the load case rather than the average.

Existing concrete covers are the harder case. Once the underside has gone soft, a coating will not save it. The repair sequence is to remove the softened layer, neutralise the surface, rebuild with a sulfate-resisting mortar, and only then apply the barrier. Skipping the first step is why so many recoated covers fail again within two seasons.

Whatever the panel, the seal and the fixings decide the outcome. EPDM gaskets, stainless bolts and a proper compression set at every hatch last. Mild steel hinges on a wet cover do not.

Material passports

Each card gives the four numbers that decide a specification. Cost is relative to PP, which sits at 1.0.

PVC0.7–0.9×
Max continuous
60°C
Wet H2S
Good up to 50% acid
Weak point
Brittle on impact, poor above 60°C
Use it for
Low-temperature lab and room extract
PP-H1.0×
Max continuous
80°C
Wet H2S
Excellent to 70% acid
Weak point
Creep under load above 70°C, soft against abrasion
Use it for
The default for odour duct below 80°C
Isophthalic FRP1.2–1.5×
Max continuous
about 65°C
Wet H2S
Acceptable, resin-limited
Weak point
Hydrolyses faster than vinyl ester in hot wet gas
Use it for
Mild duty where the budget is tight
Vinyl ester FRP1.5–2.0×
Max continuous
120°C duct, about 95°C tower
Wet H2S
Excellent. The liner carries the duty
Weak point
Liner quality at flanges and nozzles, field repair is hard
Use it for
Hot wet odour streams, tower shells, large ducts
316L3.0–4.0×
Max continuous
400°C
Wet H2S
Good while chloride stays low
Weak point
Pitting above about 200 mg/L chloride, SCC when hot
Use it for
Hot, abrasive or high-vacuum duty without chlorides
Duplex 22055–6×
Max continuous
High, chloride-dependent
Wet H2S
Good to high chloride
Weak point
Cost, and fabrication discipline at welds
Use it for
Hot brine or saline streams where 316L cracks

Duct material at a glance

Row of FRP washer towers with FRP duct runs and axial fans along a rooftop walkway
FRP towers and FRP duct on a roof. The shell and the duct share a resin system, which is why the pairing survives where a mixed-metal layout would not.
Duct material comparison for odour service
MaterialMax tempH2SO4 resistanceMax negative pressureRelative cost
PVC60°CGood to 50%about 2,000 Pa0.7–0.9×
PP-H80°CExcellent to 70%about 2,500 Pa1.0×
Vinyl ester FRP120°CExcellent to 70%about 5,000 Pa1.5–2.0×
316L400°CLimited to 50%over 10,000 Pa3.0–4.0×

One plant, three different answers

A single H2S corrosion duct material choice rarely fits a whole site. The conditions change with position, and the sensible specification follows them.

The headspace under a channel cover runs near ambient temperature and is saturated, so PP-H or vinyl ester FRP both work and the choice comes down to temperature margin. The duct from a scrubber outlet is warm and carries droplets, which pushes toward FRP with a proper mist eliminator ahead of it. The exhaust from a sludge room is warm, saturated and often carries oil aerosol, so the resin matters and the first metres of duct deserve a cleanout.

The tower shell follows its own rule. PP suits small and mid-size columns, vinyl ester FRP takes over for large diameters and outdoor sites, and 316L only belongs where the chlorides are low and the temperature is high. Mixing an FRP shell with a stainless fan is common and works, provided the transition is flanged and not welded.

The joints fail before the pipe does

Look at any failed odour duct and the hole is usually within a metre of a connection. The wall thickness was fine. The joint was not. No H2S corrosion duct material survives a bad flange.

Gaskets are the first weak point. EPDM covers hot aqueous duty to about 130°C and is the default for scrubber connections. FKM takes higher temperature and oily streams. PTFE-encapsulated gaskets cost more and handle almost anything. Nitrile hardens with heat and has no place on a hot odour line.

Bolts are the second. Carbon steel fasteners disappear in months on a wet H2S flange, and the leak starts at the bolt hole, not the gasket face. Specify stainless fasteners with an anti-seize compound, and check them at the first shutdown because a loose flange is silent until it drips.

Flange faces and pinholes A coating failure at a flange is worse than a coating failure on a straight run. The acid works sideways under the film and lifts the lining from the edge inward. That is why lined steel on a wet odour line needs inspection at the flanges first. A pinhole in a tank lining is also more dangerous than a scratch.

How to check what you have

Three checks catch most of the problems before they become a replacement. Run them on whatever H2S corrosion duct material you end up choosing.

  • Ultrasonic thickness on steel at the low points and near flanges, twice a year. Uniform loss is slow; a drop of 1 mm in one interval means pitting.
  • Visual on FRP for blistering, fibre show-through and a chalky surface, which signal liner breakdown rather than shell failure.
  • Condensate check at every drain. A drain that runs dry has blocked, and a blocked drain floods the low point.

For concrete, tap the surface with a hammer. A dull sound over a soft, pasty layer means the acid has already eaten into the cover zone. Repair means removing the softened layer, neutralising, and rebuilding with a acid-resistant mortar before any coating goes on. Painting over a soft substrate only hides the problem for one season.

Frequently asked questions

These come up on most reviews of an H2S corrosion duct material choice.

Choosing the material

Can I use 304 stainless for an odour duct?

Rarely. 304 is limited to low-chloride duty below about 60°C, and odour streams are warm, wet and often carry chlorides from the sewage itself. It also suffers chloride stress-corrosion cracking once temperature rises. 316L is the practical minimum, and even that needs a chloride check.

Is FRP better than stainless for H2S service?

For wet, chloride-bearing odour gas below about 100°C, generally yes. Vinyl ester FRP resists the acid and does not pit, and it costs less than 316L. Stainless wins when the gas is hot, abrasive or under high vacuum, or when impact damage is likely.

Which resin should the FRP use?

Vinyl ester for anything wet and warm. Isophthalic polyester is acceptable on mild, cooler duty and costs less, but it hydrolyses faster in hot wet gas. The resin, not the glass, sets the temperature limit, so the resin data sheet is the document that matters.

Failure and repair

Why did my stainless duct fail in two years?

Almost always chlorides plus heat, plus a stagnant pocket where the chloride concentrates as the water evaporates. Look for the failure at a weld, a low point or under a gasket. Crevices concentrate chlorides and start pitting before the open wall shows anything.

Can I repair a failed FRP duct in place?

Small areas can be ground back and laminated by hand, but the repair is only as good as the surface preparation and the cure. Large delamination or a failed liner at a flange is usually a spool replacement. Keep a spare spool of the most exposed section rather than a roll of mat.

How long should a coated concrete cover last?

It depends on the coating system and the film thickness, not on the concrete. A properly applied high-build system on a sound, neutralised substrate gives a long service life, but the failure mode is always a pinhole or a holiday at an edge. Test the coating for holidays before the cover goes into service, and re-test at each inspection.

Need a material selection sheet for your odour system?

Send the gas temperature, whether the stream is saturated, the measured or expected H2S level, the chloride content if you have it, and a sketch of the duct route. We will come back with an H2S corrosion duct material per section, the gasket and fastener specification, and the points to inspect first.

Request the selection sheet